Overview
The cross-cut test checks how well a thin coating holds to its surface when it is cut. It gives a grade from 0 to 5, not a force.
What the test measures
The test measures a coating's resistance to being separated from the substrate when a grid of cuts is made through it. It is used on thin films, such as paints on metal, wood and plastics.
How the test is carried out
The method is ISO 2409.
- Six parallel cuts are made through the cured film, down to the substrate.
- Six more are made at right angles, to form a lattice of small squares.
- The spacing of the cuts depends on film thickness and substrate: 1 mm, 2 mm or 3 mm.
- Loose material is removed, by brushing or with adhesive tape, as the method sets out.
- The lattice is compared with the standard's reference pictures and given a class.
How to read the result
Lower is better. Class 0 is the best result.
| Class | What the cut area looks like |
|---|---|
| 0 | Edges of the cuts are completely smooth. No square has detached. |
| 1 | Small flakes at the intersections. About 5% of the area or less is affected. |
| 2 | Flaking along edges or at intersections. More than 5%, up to about 15%. |
| 3 | Flaking along edges and on parts of squares. More than 15%, up to about 35%. |
| 4 | Large ribbons or whole squares detached. More than 35%, up to about 65%. |
| 5 | Anything worse than class 4. |
What it means in use
A coating that grades 0 or 1 stays attached around a cut or a chip. Damage stays local. A coating with poor cross-cut adhesion lifts away from a scratch, and the damaged area grows.
What the result does not tell you
The standard itself says the test is not a measurement of adhesion. It grades how the film behaves when cut. It does not give a bond strength.
The class is a visual judgement against reference pictures, so two operators can differ by a class.
The method is not suitable for films thicker than 250 µm or for textured coatings. Thick floor coatings are tested by pull-off.
As with any adhesion test, the result depends on the surface the coating was applied to. A class measured on clean steel does not carry over to a contaminated or unprepared surface.
On our product pages
Where a product has been tested, its page shows the result, the method and, where the method has one, the rating. Results published on this site come from internal testing to the stated method. They are given for technical reference and comparison.
If a figure you need is not shown, ask our technical team.


Share:
Abrasion Resistance (Taber Abrasion)
Impact Resistance (ISO 6272)